Mechanical Properties

ALLOY #3 #5 #7 #2 ZA-8 EZAC
Ultimate Tensile Strength
(psi x 10³)
41 48 41 52 54 60
Yield Strength 0.2% Offset
(psi x 10³)
- - - - 42 57
Elongation
(% In 2")
10 7 13 7 6-10 1
Shear Strength
(psi x 10)
31 38 31 46 - -
Hardness
(Brinell)
82 91 80 100 95-110 116
Impact Strength
(ft-lb)
43 38 43 35 31 -
Fatigue Strength Rotary Bend
(psi x 10³) (5 x 108 Cycles)
6.9 8.2 6.8 8.5 - -
Compressive Yield Strength
0.1 Offset (psi x 10³)
60 87 60 93 - -


Get A Quick Quote

Physical Properties

ALLOY #3 #5 #7 #2 ZA-8
Density
(lb/cu in)
.24 .24 .24 .24 .227
Melting Range
(°F)
719-728 717-727 718-728 715-734 707-759
Electrical Conductivity
(% IACS)
27 26 27 25 27.7
Thermal Conductivity
(BTU/ft-hr°F)
65.3 62.9 65.3 60.5 66.3
Coefficient Of Thermal Expansion
(68-212°F) (u in/in/°F)
15.2 15.2 15.2 15.4 12.9
Specific Heat
(BTU/lb°F)
.10 .10 .10 .10 .104
Pattern Or Die Shrinkage .006 in/in .006 in/in .006 in/in .006 in/in 1/8 in/ft   |   .007 in/in


Get A Quick Quote

Chemical Specifications (Per ASTM)

ALLOY #3 INGOT #3 CASTING #5 INGOT #5 CASTING #7 INGOT #7 CASTING #2 INGOT ZA-8 INGOT
Aluminum 3.9-4.3 3.5-4.3 3.9-4.3 3.5-4.3 3.9-4.3 3.5-4.3 3.9-4.3 8.0-8.8
Magnesium .025-.050 .02-.05 .03-.06 .03-.08 .01-.02 .005-.020 .025-.050 .015-.030
Copper .10 max .25 max .75-1.25 .75-1.25 .10 max .25 max 2.6-2.9 0.8-1.3
Iron (max) .075 .10 .075 .10 .075 .075 .075 .10
Lead (max) .004 .005 .004 .005 .002 .003 .004 .004
Cadmium (max) .003 .004 .003 .004 .002 .002 .003 .003
Tin (max) .002 .003 .002 .003 .001 .001 .002 .002
Nickel - - - - .005-.020 .005-.020 - -
Zinc Balance Balance Balance Balance Balance Balance Balance Balance